          Iron Agent

          Update time:2021-03-05
          Instructions for use of iron additives◆ UseAdjust the iron content in pure aluminum: provide the alloying element-iron in aluminum alloy.◆ WeightEach piece of iron agent weighs 500 5 grams.◆ Composition75% iron in iron◆ Consumption: Set: 1000 kg …

          Service hotline

          +86-0516-83248188
          • Product Details

          Instructions for use of iron additives

          ◆ Use

          Adjust the iron content in pure aluminum: provide the alloying element-iron in aluminum alloy.

          ◆ Weight

          Each piece of iron agent weighs 500 ± 5 grams.

          ◆ Composition

          75% iron in iron

          ◆ Consumption: Set: 1000 kg of molten aluminum, 0.2% iron in molten aluminum (analysis after melting). If you want to adjust the iron in molten aluminum to 0.5%, then: (0.5-0.2) 96x1000÷90%=6-47.6kG≈48kG (limited to 96 pieces) iron agent

          ◆ In the formula

          75% is the iron content in the iron agent, and 90% is the iron recovery rate in the iron agent.

          ◆ How to use

          After the charge is completely melted, stir vigorously and take samples for analysis. Calculate the amount of iron added based on the analysis results. When the temperature of the molten aluminum is 745-755°C, remove the scum on the surface of the molten aluminum, and evenly put the iron agent into the molten pool (you also need to add manganese. When the pot agent, you can add it at the same time. Let it stand for 20-30 minutes, Then vigorously stir for 5 minutes, and then stand for 5-10 minutes, sample and analyze. After the ingredients are qualified, it can be transferred to the next process.

          ◆ Explanation

          This product is stable, reliable, and easy to use. It is non-toxic and produces flame and trace smoke after being added to the molten pool. Properly control the adding temperature and standing time, and the degree of stirring is the key to improving the recovery rate. Pay attention to moisture-proof during storage, and oxidize and pulverize after being wet.

          From the production date, the shelf life is ten months.


          精品国产精品国在线_国产真实乱子伦清晰对白_亚洲av偷拍无码专区_2020年黄色视频最新网站 亚太影院 柯西贝尔-游戏赚网 精品超清无码视频在线观看 久久人妻无码一区二区三区 亚洲AⅤ一级无码

          <sup id="9hl9x"><rp id="9hl9x"></rp></sup>
            <object id="9hl9x"><button id="9hl9x"><noscript id="9hl9x"></noscript></button></object>
              <dfn id="9hl9x"><b id="9hl9x"><span id="9hl9x"></span></b></dfn>
                  <menuitem id="9hl9x"><p id="9hl9x"><u id="9hl9x"></u></p></menuitem>
                  无码人妻久久一区| 久久久久人妻乱淫视频系列| 国产乡下妇女做爰视频| 亚洲第一极品精品无码| 91综合在线| 国产精品系列在线| 国产a级免费无码播放| 免费国产va在线观看| 国产日韩精品无码一区二区三区| 一区二区国产欧美在线视频| 国产亚洲欧美日韩综合一区在线观看| 国产午夜精品久久| 欧美日韩国产一区二区三区在线| 92看片淫黄大片看国产片| 国产成人_综合_亚洲_国产| 无码人妻精品一区二区三区97| 91视频久久| 国产日韩欧美在线在线视频| 大屁股国产白浆一二区|